EA-40®

EA-40®

EA-40®为未填充低粘度透明琥珀色环氧树脂粘合剂,易于薄膜摊铺,固化后几乎透明。EA-40®操作时间长,室温下24小时内固化,具有良好的机械和电气性能。体积混合比为1:1。当以体积比为2A:1B混合时,EA-40®具有更高的耐热性和改善的物理性能。EA-40®具有多功能性,可用于许多不同的装配和修理应用场合,从电子灌封到珠宝装配到维修管道装置。作为极好的层压树脂,EA-40®已被弓箭制造商所知。EA-40®具有高度防潮的粘合性,符合联邦规范MMM-A-188,III型的性能要求。

特征

说明

Safety - Use in a properly ventilated area (“room size” ventilation). Wear safety glasses, long sleeves and rubber gloves to minimize contamination risk.
 

Store and use material at room temperature (73°F/23°C). This product has a limited shelf life and should be used as soon as possible.

A clean, dry surface is a necessary prerequisite for adhesive bonding. Adhesives will stick to either the surface of which a bond is desired or to that film of extraneous material directly on that surface. Rarely can a structural adhesive penetrate through surface contaminants to provide an optimum bond on an unclean surface.

Porous materials are simple to bond, provided they are dry. The surface should be sanded till clean and free from dust. Non-porous surfaces, such as found on metal and plastic materials, should be degreased, dried and roughened by sanding, sandblasting or chemical etching. The etched or sandblasted surfaces should be covered within a few hours of treatment to prevent contamination.

Handlers should wear clean cotton gloves to prevent body oils from contaminating the clean surfaces.

Epoxy adhesives do not perform well on metals such as nickel, chromium, tin or zinc nor on soft thermoplastics like polyethylene.

Because no two applications are quite the same, a small test application to determine suitability for your project is recommended if performance of this material is in question.


MEASURING & MIXING - Measure equal amounts of Parts A and B (or 2A:1B) by volume into a clean mixing container. Mixing tools and containers should be clean and made of metal, glass or plastic. After dispensing required amount of Parts A and B into mixing container, mix thoroughly for 3 minutes making sure that you scrape the sides and bottom of the mixing container several times.


Application - Apply to prepared surface and let cure for 24 hours. Applying mild heat will cure EA-40® faster – 150°F/65°C for 6 hours.

Post Curing - After EA-40® has cured at room temperature, heating the epoxy to 150° F (65° C) for 4 to 8 hours will increase physical properties and performance. Let cool to room temp. before moving bonded substrates, machining, etc.

To Attain Maximum Heat Distortion Temperature - let cure for 24 hours at room temperature, heat cure for 2 hours at 250°F (122°C).

At mix ratio 1A:1B – HDT will be 163°F (73°C).

At mix ratio 2A:1B – HDT will be 217° F (103 °C)

介绍产品制作工艺的文章