Accel-T™

Accel-T™

Accel-T™ 为单组分添加剂,可缩短Smooth-On锡固化硅胶的固化时间。与添加量成正比,固化时间从一晚到几个小时。在添加A组分前,Accel-T™按B组分的百分比添加。
重要提示:操作时间与Accel-T™的添加量成正比地大幅降低。硅胶的粘度也会增加。快速混合、抽真空和浇注。

特征

说明

IMPORTANT: Thoroughly Pre-mix Accel-T™ with Part B before adding Part A. Adding Accel-T® will reduce the library life of tin-cured silicone rubber in proportion to the amount added.
 

Safety – Use in a properly ventilated area ("room size" ventilation). Wear safety glasses, long sleeves and rubber gloves to minimize contamination risk. Store and use all products at room temperature. This product has a limited shelf life and should be used as soon as possible. Wear gloves and eye protection to minimize risk of contamination.

All components must be measured using an accurate gram scale.

1. Determine the total amount of rubber required for your application. Calculate the correct amounts of Part A, Part B and Accel-T® in advance.

2. Weigh out the required amount of Part B

3. Weigh out and add the required amount of Accel-T™ as a percentage of the Part B. Mix Part B and Accel-T® thoroughly.

4. Weigh out and add the required amount of Part A.

5. Mix thoroughly, eliminating all color streaks from the mixture.

6. Pour mixture into new, clean mixing container and mix again.

7. Vacuum material (29 h.i.g. mercury) as directed on the silicone rubber technical bulletin.

8. Pour rubber into containment field, let rubber rise over model.

Because no two applications are quite the same, a small test application to determine suitability for your project is recommended if performance of this material is in question.

IMPORTANT: Working time (pot life) is drastically reduced in proportion to the amount of Accel-T™ added. Viscosity of rubber will also increase. Mix, vacuum and pour quickly.